Chemistry › Section Q · Electrochemistry › Topic Q.6

Corrosion and electrolysis

Left alone, iron in damp air slowly runs a galvanic cell that eats it away. Push electrons the other way with a power supply and you can split water, refine metals and plate a spoon with silver, all in amounts you can calculate from the current and the time.

Redox we fight and redox we force

Corrosion is the gradual destruction of a metal by spontaneous redox reactions with its surroundings, usually oxygen and water. Rust on iron, the dark tarnish on silver and the green coat on copper roofs are all corrosion. It is costly: one widely quoted industry study estimated the global cost at about $2.5 trillion a year. In electrolysis, by contrast, a power supply forces a non-spontaneous redox reaction, producing aluminium and chlorine, recharging batteries and plating metals. Both are governed by the same reduction potentials used for galvanic cells.

How iron rusts

A drop of water on iron sets up a tiny galvanic cell on the metal's surface. Where oxygen is scarce, near the centre of the drop, iron acts as the anode: \(\mathrm{Fe(s) \rightarrow Fe^{2+}(aq) + 2e^-}\). Electrons flow through the metal itself to regions with more oxygen, near the drop's edge, which act as the cathode:

\mathrm{O_2(g) + 2H_2O(l) + 4e^- \rightarrow 4OH^-(aq)}\,,

E° = +0.40 V. With Fe²⁺/Fe at −0.44 V, the cell has \(E^\circ = +0.84\) V. The \(\mathrm{Fe^{2+}}\) ions are then oxidised further by air to a hydrated iron(III) oxide, \(\mathrm{Fe_2O_3 \cdot xH_2O}\), which is rust. Dissolved salt makes the water a better electrolyte, so cars rust faster on salted roads.

Why rust keeps spreading

Rust is porous and flakes away, exposing fresh iron, so corrosion continues. Aluminium is more easily oxidised than iron, yet it lasts well outdoors, because a thin, tightly bonded aluminium oxide layer seals its surface. Copper's green patina of basic copper carbonates and sulfates also protects the metal beneath. Protection by such a film is called passivation. Stainless steel uses the same idea: it contains at least 10.5 percent chromium, which forms an invisible, self-repairing chromium(III) oxide film.

Keeping metal safe

Most protection either keeps water and oxygen away or arranges for another metal to corrode instead. Paint, oil and plastic coatings are barriers, but they work only while unbroken. Galvanising coats steel with zinc. Zinc is a barrier too, and if the coating is scratched, zinc, with E° = −0.76 V, is oxidised in preference to iron, so the exposed steel is still protected. Tin plating on food cans works differently: tin, at −0.14 V, lies above iron in the table, so at a scratch the iron becomes the anode and corrodes faster than if it were bare.

Sacrificial anodes

Cathodic protection makes the iron the cathode of a deliberate galvanic cell. A block of a more easily oxidised metal, usually magnesium, zinc or an aluminium alloy, is wired or bolted to the steel. That block becomes the anode and slowly dissolves, while oxygen is reduced on the steel, which only passes electrons along. Because it is used up on purpose, it is called a sacrificial anode, and it is replaced as it wears. Such anodes protect ships' hulls, buried pipelines and the steel tanks of hot-water heaters, which contain a magnesium or aluminium anode rod.

Worked example: choosing a sacrificial anode

Which of magnesium, copper, tin and zinc could protect a buried steel pipe? 1. The metal must be oxidised in preference to iron, so its reduction potential must be below that of \(\mathrm{Fe^{2+}/Fe}\), −0.44 V. 2. Compare: Mg −2.37 V and Zn −0.76 V lie below; Sn −0.14 V and Cu +0.34 V lie above. 3. Magnesium and zinc qualify. For zinc joined to iron with oxygen reduced at the iron, \(E^\circ = +0.40 - (-0.76) = +1.16\) V, larger than the 0.84 V of iron's own corrosion cell, so zinc is oxidised first. 4. Check: copper or tin would make the iron the anode and speed up its corrosion, the opposite of what is wanted.

Electrolytic cells

An electrolytic cell uses an external power supply to drive a reaction with a negative cell potential. The supply must provide more than the size of that potential, plus an extra amount called the overpotential that real electrodes need for the reaction to run at a useful rate. Oxidation still happens at the anode and reduction at the cathode, but the signs change. The supply pulls electrons out of the anode, making it positive, and pushes them into the cathode, making it negative: the reverse of a galvanic cell.

Molten salts, water and brine

Molten sodium chloride gives sodium at the cathode, \(\mathrm{Na^+ + e^- \rightarrow Na}\), and chlorine at the anode, \(\mathrm{2Cl^- \rightarrow Cl_2 + 2e^-}\). Using aqueous potentials as a rough guide, \(E^\circ = -2.71 - 1.36 = -4.07\) V, so over 4 V is needed. Water splits into hydrogen at the cathode and oxygen at the anode, 2 : 1 by volume, needing more than 1.23 V; an electrolyte such as sodium sulfate is added so it conducts. In salt water, or brine, water is reduced instead of sodium ions, giving \(\mathrm{H_2}\) and \(\mathrm{OH^-}\), while chlorine forms at the anode, because oxygen needs a large overpotential. The net reaction is

\mathrm{2Cl^- + 2H_2O \rightarrow Cl_2 + H_2 + 2OH^-}\,,

the chlor-alkali process.

Counting electrons: charge, current and time

Every electron through the circuit drives one electron's worth of reaction, so electrolysis can be calculated exactly. Current is charge per second, \(\mathrm{1\ A = 1\ C\ s^{-1}}\), so a steady current I for time t moves a charge

Q = It

with t in seconds. Dividing by the Faraday constant gives moles of electrons, \(n_{e^-} = Q/F\). The half-reaction then converts electrons to product: \(\mathrm{Ag^+ + e^- \rightarrow Ag}\) needs 1 mol of electrons per mole of silver, and \(\mathrm{Cu^{2+} + 2e^- \rightarrow Cu}\) needs 2. In electroplating, the object to be coated is the cathode, and a bar of the plating metal is the anode, which dissolves to replace the ions used.

Worked example: copper plating

A current of 2.50 A passes for 45.0 min through copper(II) sulfate solution. What mass of copper is plated? 1. Time in seconds: \(45.0 \times 60 = 2700\) s. 2. Charge: \(Q = It = 2.50 \times 2700 = 6750\) C. 3. Electrons: \(6750 \div 96{,}485 = 0.06996\) mol. 4. Copper: two electrons per atom, so \(0.06996 \div 2 = 0.03498\) mol. 5. Mass: \(0.03498 \times 63.55 = 2.22\) g. 6. Check: about 0.07 mol of electrons makes about 0.035 mol of copper, roughly 2.2 g. The steps in reverse give a time: depositing 1.00 g of silver at 0.750 A takes \(\frac{(1.00/107.87) \times 96{,}485}{0.750} = 1.19 \times 10^3\) s, about 19.9 min.

Common mistakes to avoid

First, leaving time in minutes or hours in \(Q = It\); it must be in seconds. Second, forgetting to divide by the electrons per atom, 2 for copper and 3 for aluminium. Third, carrying galvanic sign conventions into electrolysis: there the anode is positive. Fourth, expecting sodium metal from salt water; water is reduced instead. Fifth, choosing a sacrificial anode that lies above iron in the table, such as copper or tin. Sixth, thinking any coating protects once scratched: zinc does, tin does not.

Key takeaways

Corrosion is spontaneous redox: iron is the anode, oxygen is reduced at the cathode, and salt water speeds it up. Passivating oxide films protect aluminium, copper and stainless steel; rust does not. Galvanising and sacrificial anodes of magnesium or zinc work because those metals are oxidised in preference to iron. Electrolysis forces non-spontaneous reactions; the anode is still oxidation but is now positive. Charge is current times time, \(Q = It\); divide by F for moles of electrons, then use the half-reaction to find moles and mass of product.

Flashcards

Flashcard

Corrosion

Destruction of a metal by spontaneous redox reactions with its surroundings

Rust, tarnish and patina.

Test your understanding

Question 1 of 5

A current of 3.00 A passes through copper(II) sulfate solution for 30.0 min. What mass of copper is deposited?

Question 2 of 5

Which metal could serve as a sacrificial anode to protect a steel pipe?

Question 3 of 5

In an electrolytic cell, which statement about the anode is correct?

Question 4 of 5

What forms at the cathode when concentrated aqueous sodium chloride is electrolysed?

Question 5 of 5

Why does iron rust faster in salt water than in pure water?